Analysis of PCB Negative Deformation in PCB Process
29Nov
Jeff 0條評論

Analysis of PCB Negative Deformation in PCB Process

The following is an analysis of PCB negative deformation in PCB process

1、 The causes and solutions of film deformation are as follows:

reason:

(1) Temperature and humidity control failure

(2) The temperature rise of the exposure machine is too high

resolvent:

(1) Generally, the temperature is controlLED at 22 ± 2 ℃ and the humidity is 55% ± 5% RH.

(2) Exposure machine with cold light source or cooling devICe and continuous replacement of backup film

pcb board

2、 Process method of PCB negative deformation correction:

1. Under the condition of mastering the operation technology of the digital programming instrument, first install the negative film to compare with the drilling test plate, measure its length and width, lengthen or shorten the hole position according to the size of the deformation on the digital programming instrument, and use the drilling test plate after lengthening or shortening the hole position to match the deformed negative film, so as to avoid the tedious work of splicing the negative film, and ensure the integrity and accuracy of the graphics. This method is called "hole location change method".

2. In view of the physical phenomenon that the negative film changes with the change of ambient temperature and humidity, take out the negative film in the sealed bag before copying the negative film, and hang it in the air for 4-8 hours under the working environment to deform the negative film before copying, so that the deformation of the copied negative film will be very SMAll. This method is called "hanging in the air method".

3. For graphics with SIMple lines, large line width and spacing, and irregular deformation, the deformed part of the negative film can be cut off and compared with the hole position of the drilling test plate, and then copied, which is called "splicing method".

4. This method is called "pad overlap method", which uses holes on the test board to enlarge the pad to remove heavy and deformed circuit pieces to ensure the minimum ring width technical requirements.

5. This method is called "mapping method", in which the figures on the deformed negative film are scaled up and remapped for plate making.

6. The CAMera is used to enlarge or reduce the deformed figure, which is called "photographic method".

3、 Precautions for relevant methods:

1. Splicing method:

Application: The PCB circuit is not too dense, and the film deformation of each layer is inconsistent; It is especially suitable for the deformation of resistance welding negative film and multilayer power supply layer negative film;

Not applicable: negative film with high wire density, line width and spacing less than 0.2mm;

Precautions: The conductor shall be cut as little as possible without damaging the bonding pad. Pay attention to the correctness of the connection relationship of PCB boards when editing after splicing copies.

2. Change hole location method:

Application: The deformation of each layer of negative film is consistent. This method is also applicable to films with dense lines;

N/A: The negative film has uneven deformation, especially local deformation.

Precautions: After using the programmer to lengthen or shorten the hole position, the hole position exceeding the tolerance shall be reset.

3. Hanging method:

Applicable; Negative film that has not been deformed and prevented from deformation after copying;

Not applicable: deformed negative film.

Precautions: Hang the negative film in a ventilated and dark (safe) environment to avoid pollution. Ensure that the temperature and humidity of the hanging place are consistent with that of the operation place.

4. PCB pad overlap method:

Applicable: the graphic lines are not too dense, and the line width and spacing are greater than 0.30mm;

Not applicable: In particular, users have strict requirements on the appearance of printed circuit boards;

Note: The pad is elliptical after overlapping copies. Halo and deformation of line and disk edges after overlapping copy.

5. Photographic method:

Application: The deformation ratio in the length and width directions of the negative film is consistent. When it is inconvenient to drill the test plate again, it is only applicable to silver salt negative film.

N/A: PCB negative is deformed inconsistently in the length and width directions.

Precautions: The focus should be accurate when taking pictures to prevent line deformation. There is a lot of film loss. Generally, you need to debug many tiMES to get a satisfactory PCB circuit pattern.

In a word, this paper is mainly about the analysis of PCB negative deformation in PCB process

點擊
然后
聯系
主站蜘蛛池模板: 国产色综合天天综合网| 中文字幕丰满乱子无码视频| 国语对白做受xxxxx在线中国| 欧美性猛交aaaa片黑人| 亚洲欧美精品一中文字幕| 青青草无码精品伊人久久7| 天天狠天天添日日拍捆绑调教| 99国产精品国产精品九九| 十八禁免费观看| 狠狠色丁香五月综合婷婷| 天天做天天躁天天躁| 69国产成人精品午夜福中文| 国产女人高潮抽搐叫床视频| 国产精品美女久久久网站| 亚洲国产一区二区三区波多野结衣| 人妻精品动漫h无码中字| 97久久超碰成人精品网页| 又大又粗又爽免费视频a片| 国产 高潮 抽搐 正在播放| 97国产露脸精品国产麻豆| 国产精品国产三级国产av麻豆| 亚洲乱码日产精品bd在线观看| 中文字幕久久熟女蜜桃| 国产系列丝袜熟女精品网站| AI做受???高潮AAAA视频| 麻豆一区二区在我观看| 国产偷窥熟女精品视频大全| 2021年精品国产福利在线| 久久成人影院精品777| 末成年女av片一区二区丫| 国产成年无码av片在线| 久久久久国产精品嫩草影院| 亚洲已满18点击进入在线看片| 夜夜高潮夜夜爽夜夜爱爱一区| 国产在线视频一区二区三区| 亚洲成a人片在线观看www| 国产精品一区二区久久精品| 欧美亚洲一区二区三区| 欧美黑人又粗又大又爽免费| 亚洲熟女少妇一区二区| 老湿机69福利区无码|